CONATHANE EN-5317 Polyurethane Encapsulant

Harmonization Code : 3909.20.00.90 | Amino-resins, phenolic resins and polyurethanes, in primary forms : Melamine resins : Other

CONATHANE EN-5317 Polyurethane Encapsulant

Main features

  • 300 cP Mixed Viscosity
  • 1:1 Controlled Mixing
  • Clear Polyurethane for Potting and Bonding

Product Description

CONATHANE EN-5317 is an unfilled, two-component polyurethane system for potting, encapsulating, and bonding electrical and electronic assemblies. Part A urethane prepolymer and DP32127 Part B curative mix at 100:97 by weight or 1:1 by volume. The mixed system has a typical initial viscosity of 300 cP and a 10-15 minute work life at 25 C. Documented applications include electrical potting, electronic encapsulation, and adhesive bonding. Use either 7-10 days at 25 C or 16 hours at 80 C.

Key features

  • Flow and dispensing: Low initial mixed viscosity of 300 cP at 25 C.
  • Mix ratio: Cartridge-friendly 1:1 mix ratio by volume.
  • Application fit: Clear polyurethane for potting, encapsulation, and bonding.

Applications

  • Electrical potting
  • Electronic encapsulation
  • Adhesive bonding

Technical Specifications

General Properties
Component System
2 Part (Urethane Prepolymer | Curative)
Physical Properties
Tack-Free Time
10 minutes
Mechanical Properties
Elongation
200 %

Additional Information

Two-Component Polyurethane Potting Compound

CONATHANE® EN-5317 DP32127

CONATHANE® EN-5317 DP32127, formerly CONAP EN-5317, is a two-component, unfilled polyurethane potting and encapsulating compound used for electrical and electronic assemblies exposed to challenging environmental conditions involving high ambient temperature, humidity, and exposure to sunlight.

The material is mixed at a 1:1 ratio by volume (Part A to Part B) before application. It supports hand-mix bench processing, cartridge dispensing, meter-mix bench processing, and meter-mix vacuum processing. After application, the material can be cured for 7 to 10 days at 25°C or for 16 hours at 80°C.

1:1 mix ratio by volume 300 cP initial mixed viscosity 10–15 min work life at 25°C UV-stable polyurethane system
Safety data sheets by component

CONATHANE® EN-5317 DP32127 has separate safety data sheets for Part A and Part B. The Safety data sheet button above opens the Part A document.

CONATHANE EN-5317 DP32127 two-component polyurethane potting and encapsulating compound
Polyurethane potting and encapsulating compound for electrical and electronic assemblies
Key features

Low-viscosity potting for electronic assemblies

  • 1:1 mix ratio by volume: Cartridge-friendly dispensing supports convenient mixing and processing.
  • Low viscosity: Initial mixed viscosity of 300 cP helps material flow into assemblies and components.
  • UV-stable polyurethane system: Suitable for electronic assemblies exposed to sunlight, humidity, and elevated temperatures.
  • Environmental resistance: Documented thermal shock, heat aging, and humidity aging test results support evaluation for challenging conditions.
  • Electronic assembly protection: Formulated for electronic circuits, components, and assemblies requiring protection from humidity, temperature exposure, and outdoor environments.
Processing summary

Two-component mixing and curing

Components: EN-5317 Part A urethane prepolymer and EN-5317 DP32127 Part B curative.
Mix ratio: 100:100 parts by volume or 100:97 parts by weight (Part A to Part B).
Initial mixed viscosity: 300 cP at 25°C / 77°F.
Work life: 10–15 minutes at 25°C / 77°F.
Thin-film tack-free time: 10 minutes at 80°C / 176°F.
Curing options: 7–10 days at 25°C / 77°F or 16 hours at 80°C / 176°F.
Applications

Highly recommended for

CONATHANE® EN-5317 DP32127 is formulated for electronic circuits, components, and assemblies requiring protection from humidity, temperature exposure, and outdoor environments.

Electrical Assembly Potting
Potting of electrical assemblies requiring protection from environmental exposure.
Electronic Component Encapsulation
Encapsulation of electronic components and assemblies.
Adhesive Applications
Adhesive applications for electronic systems.
Environmental Exposure
Electronic assemblies exposed to heat, humidity, and sunlight.
Technical specification

Typical Properties of Material as Supplied

Property CONATHANE®
EN-5317 Part A
Urethane Prepolymer
CONATHANE®
EN-5317 DP32127 Part B
Curative
Conditions
Viscosity 1,000 cP 220 cP 25°C / 77°F
Specific Gravity 1.06 1.03 25°C / 77°F
Appearance Clear Clear —
Mix Ratio — Parts by Weight 100 97 Parts by weight
Mix Ratio — Parts by Volume 100 100 Parts by volume
Flashpoint > 94°C
> 201°F
> 94°C
> 201°F
ASTM D93

Mix ratios refer to Part A and Part B respectively. The ratio by weight differs from the ratio by volume.

Mixed material properties

Typical Properties of Mixed Materials

Property Value Conditions
Mixed Viscosity (Initial) 300 cP 25°C / 77°F
Work Life 10–15 mins 25°C / 77°F
Tack Free (Thin Film) 10 mins 80°C / 176°F
Cured material properties

Typical Physical Properties

Specimens cured for 16 hours at 80°C / 176°F.

Property Value Test Method Condition
Shore Hardness A 70 ASTM D2240 25°C / 77°F
Tensile Strength 2,200 psi ASTM D412 25°C / 77°F
Ultimate Elongation 200% ASTM D412 25°C / 77°F
Tear Strength 110 pli ASTM D624 25°C / 77°F
Linear Shrinkage < 0.1% MIL-M-24041C —

Lap Shear Properties

Substrate Primer Condition Lap Shear Value
Steel Without primer 775 psi
Steel Primed with CONAP® AD-1146 790 psi
Aluminum Without primer 310 psi
Aluminum Primed with CONAP® AD-1146 670 psi
Environmental performance

Mechanical Aging Tests

CONATHANE® EN-5317 DP32127 passed 10 cycles of thermal shock testing from -70°C to 130°C under MIL-I-16923E. Separate heat aging and humidity aging tests recorded tack-free hardness results after 1,000 hours of exposure under the stated conditions.

Property Value / Observation Test Method Condition
Thermal Shock Pass 10 cycles MIL-I-16923E -70°C to 130°C
Heat Aging Shore A 87
Clear, no tack
— 1,000 hours at 70°C / 158°F
Humidity Aging Shore A 67
Slightly yellow, no tack
— 1,000 hours at 85°C / 85% RH

The values above describe the stated aging test results and conditions. The thermal shock test range is not presented as a continuous operating-temperature rating.

Processing options

Application Methods

CONATHANE® EN-5317 DP32127 supports the following potting and casting methods.

Hand-mix Bench
Potting / Casting
Cartridge-dispensed
Potting / Casting
Meter-mix Bench
Potting / Casting
Meter-mix Vacuum
Potting / Casting
Application guidance

Application and Curing Schedule

1. Measure and Mix
  1. Measure EN-5317 Part A and EN-5317 DP32127 Part B according to the specified mix ratio.
  2. Pour both components into a clean metal or glass container.
  3. Mix thoroughly using a metal or glass stirrer until a uniform blend is achieved.
2. Degas
  1. Ensure the container is large enough to accommodate any frothing during degassing.
  2. Degas the mixture at room temperature under a vacuum greater than 27 in. Hg until entrapped air is removed.
3. Cure

Use one of the following curing schedules:

  • 7–10 days at 25°C / 77°F, or
  • 16 hours at 80°C / 176°F.

Start the cure time only after the material reaches the specified cure temperature. Adjust cure conditions as needed to achieve the desired performance for the application.

Additional information

Shelf Life, Transportation & Storage

Storage Conditions

Store at 20–30°C / 68–86°F in a dry, controlled environment out of direct sunlight.

This material should be suitable for use when stored under these conditions in its original sealed containers for twelve (12) months from the date of shipment. Cartridge packaging may adjust product shelf life.

Failure to store the product as recommended may lead to deterioration in product performance.

Moisture Sensitivity and Container Handling

The product is sensitive to moisture and atmospheric humidity. Containers, once opened, should be used immediately or blanketed with dry air or nitrogen before resealing.

Component Safety Documentation

Refer to the separate safety data sheets for Part A and Part B when reviewing handling and safety information.

Part A Crystallization

CONATHANE® EN-5317 Part A may crystallize upon storage or during shipment. If crystallization has occurred, heat to 60°C, mix thoroughly, and cool to room temperature before processing.

Industry applications

Used for Agricultural Controllers

Agricultural controllers are used for modern farming systems such as irrigation control, autonomous equipment, and crop monitoring devices. These electronic assemblies are constantly exposed to moisture, dust, contaminants, temperature changes, and other harsh environmental conditions that can affect reliability.

CONATHANE® EN-5317 DP32127 can be used for potting and encapsulation of electrical and electronic assemblies of these agricultural controllers, providing protective layers around sensitive components. This helps reduce exposure to environmental conditions and supports reliable operation in demanding agricultural environments.

Smart agriculture view showing a person using a tablet to manage farming operations. Alongside connected visuals of real-time crop monitoring, automated machinery, environmental sensing, sustainable practices, and efforts to improve crop yields and food production efficiency.
Industry applications

Used for Automotive Electronics

Automotive electronics and sensors are exposed to challenging environmental conditions, including moisture, dust, chemicals, vibration, and high ambient temperature. Electronic components continue to increase in both electric and conventional vehicles, making protection of these assemblies important for maintaining reliability, performance, and a long service life.

CONATHANE® EN-5317 DP32127 can be used for potting and encapsulation of electrical and electronic assemblies of electronic control modules, sensors, and circuit boards found in automotive applications. The material helps shield sensitive components from environmental exposure and mechanical stress, supporting the durability and reliability of automotive electronic systems.

Modern white car with labeled automotive sensors and electronic components, including cameras, radar, GPS, ultrasonic sensors, pressure sensors, and power electronics.
Industry applications

Used for LED Lighting

A vertical infographic for LED signage technology. Three icons at the top represent communication, direction, and durability. Four panels in the middle depict outdoor environmental conditions: sunlight, rain, dust, and temperature extremes. Three icons at the bottom represent consistent brightness, accurate color uniformity, and reliable performance, highlighting the factors that support dependable LED display operation.

LED signage, controllers, and drivers must provide consistent performance while operating in environments that are exposed to moisture, temperature fluctuations, and prolonged outdoor exposure. Protecting electronic assemblies is critical to maintaining brightness, reliability, and long-term system performance.

CONATHANE® EN-5317 DP32127 can be used for potting and encapsulation of electrical and electronic components within LED signage and controller systems. This creates a protective barrier around sensitive circuitry, helping reduce environmental exposure and supporting reliable operation in LED lighting applications.

Industry applications

Used for Smart Meters

Three-panel infographic showing gas, water, and electric meters with corresponding utility icons and modern technical design elements.

Smart electricity, water, and gas meters rely on electronic assemblies that must operate reliably under varying environmental conditions. Moisture exposure and temperature fluctuations can affect sensitive components, potentially compromising meter performance and measurement accuracy.

CONATHANE® EN-5317 DP32127 can be used to encapsulate printed circuit boards and electronic components within smart meters, including inductors, coils, and voltage regulators. By forming a protective barrier around these assemblies, the material helps reduce exposure to environmental conditions that could affect their long-term reliability.

ELANTAS Materials Solutions for Smart Meters
Next steps

Review CONATHANE® EN-5317 DP32127 for your potting and encapsulation application

Share your electrical or electronic assembly type, potting or casting method, mixing requirements, cure conditions, and environmental exposure requirements when reviewing CONATHANE® EN-5317 DP32127 for your application.

Leading Brands Trust in Our Products and Services

Products that Perform| Knowledge that Serves| Service that Delivers